Effect of Sandblasted Surface Roughness of Titanium Alloy on the Bond Strength and Fatigue Life of CuNiIn Coatings
摘要
热喷涂前的喷砂工艺是必要且非常重要的步骤,直接决定热喷涂涂层的结合力等关键性能,过喷造成材料表面损伤、变形,少喷则氧化层去除不彻底,涂层的结合力差,因此采用何种喷砂工艺,在什么样的粗糙度下才能制备较好的热喷涂涂层,需要开展工艺探索.因此,本研究采用6 种喷砂工艺在 TC21 钛合金表面形成6 种不同的表面形貌与粗糙度(2.18~7.50 μm),然后通过相同的超音速火焰喷涂工艺制备 CuNiIn 涂层,研究了涂层的粗糙度、结合强度、残余应力与疲劳寿命等性能特征.结果表明:当基体表面粗糙度为 6.75 μm 时,涂层具有最优的结合强度(54.93 MPa)和排名第六的抗疲劳性能(84.99×105 次),相当于原基体的91.88%;当基体表面粗糙度为6.37 μm 时,涂层具有排名第二的结合强度(53.81 MPa)和排名第五的抗疲劳性能.当基体表面粗糙度从6.75 μm 升高到7.50 μm 时,涂层的结合强度和疲劳寿命下降明显,下降的主要原因是基体尖角处尖锐性缺口较多易形成应力集中,存在微裂纹,界面处易形成孔隙,棕刚玉易嵌入基体中以及超音速火焰喷涂制备的涂层存在较大的拉应力.超音速火焰喷涂前将基体表面粗糙度控制在6.37 μm 或6.75 μm 较好,制备的涂层具有较好的结合强度和较高的疲劳寿命,也就是说6.37 μm、6.75 μm 的表面粗糙度情况下,结合强度与疲劳寿命方面平衡得较好,从工程角度来说6.37~6.75 μm 区间能获得较好的性能,可作为工业产品应用.
Sandblasting is a necessary and critical step before thermal spraying because it directly determines key properties such as coating bond strength.Excessive sandblasting can damage and deform the material surface,whereas insufficient sandblasting may leave the oxide layer incompletely removed and result in poor coating adhesion.Therefore,the appropriate sandblasting process and the surface roughness required to produce a high-quality thermally sprayed coating need to be determined.In this study,six sandblasting processes were used to produce six dif-ferent surface morphologies and roughness levels(2.18-7.50 μm)on TC21 titanium alloy.CuNiIn coatings were then deposited under identical conditions by high-velocity oxy-fuel(HVOF)spraying,and their roughness,bond strength,residual stress,and fatigue life were evaluated.
When the substrate surface roughness was 6.75 μm,the coating exhibited the highest bond strength(54.93 MPa)and the sixth-best fa-tigue performance(84.99×105 cycles,equivalent to 91.88%of that of the uncoated substrate).At a substrate surface roughness of 6.37 μm,the coating exhibited the fifth-highest bond strength(53.81 MPa)and the fourth-best fatigue performance.When substrate roughness increased from 6.75 to 7.50 μm,coating bond strength and fatigue life decreased markedly.This decrease was attributed to stress concentrations and mi-crocracks caused by numerous sharp notches at substrate asperities,interfacial pores,embedding of brown fused alumina in the substrate,and high tensile residual stress in the HVOF-sprayed coating.
Controlling substrate surface roughness to 6.37 μm or 6.75 μm before HVOF spraying produced coatings with favorable bond strength and fatigue life.From an engineering perspective,a surface roughness range of 6.37-6.75 μm provides a good balance between these properties and is suitable for industrial applications.