军事知识服务平台
EM2高速钢冲压模具早期失效研究
Study on early failure of EM2 high-speed steel stamping dies
摘要 本文针对某冷冲压生产线中服役不足 1 万冲次即发生断裂的 EM2 高速钢模具,采用化学成分检测、硬度测试、低倍组织观察、金相分析、扫描电子显微镜断口分析,以及有限元模拟相结合的方法,系统解析其失效原因.研究结果表明:失效模具化学成分与硬度均符合国家标准要求,排除材质偏差与热处理异常的直接影响;模具内部存在 2~3 级带状碳化物偏析,晶界处有粗大 M6C型共晶碳化物呈近网状分布,破坏了基体组织连续性;模具尖角处的几何应力集中与组织缺陷相叠加,在循环交变载荷作用下诱发疲劳裂纹萌生,碳化物偏析为裂纹扩展提供了优先路径,锻造夹层则加速了失效进程,最终导致模具发生早期脆性断裂.
Abstract:
An EM2 high-speed steel mold fractured after less than 10 000 strokes in a cold stamping production line was systematically investigated.A combined approach was adopted for failure analysis,including chemical composition detection,hardness testing,macrostructure observation,metallographic analysis,scanning electron microscope fracture analysis and finite element simulation.The results show that the chemical composition and hardness of the failed mold both meet the requirements of national standards,thus the direct impacts of material non-conformity and abnormal heat treatment can be eliminated.There are grade 2-3 banded carbide segregation inside the mold,and coarse M6C eutectic carbides distribute in a near-net shape at grain boundaries,which destroys the continuity of the matrix structure.The geometric stress concentration at the sharp corner of the mold is superimposed with structural defects,which induces the initiation of fatigue cracks under cyclic alternating load.Carbide segregation provides a preferential path for crack propagation,and forging interlayers accelerate the failure process,which ultimately leads to the early brittle fracture of the mold.
刊 名 模具技术 ISTIC
年,卷(期): 2026, (4)
分类号: TG115.21 TG315.2
机标分类号: TG142.45 TG385.2 TH117
在线出版日期: 2026年10月19日
基金项目: NCZYDXKY2025122506:南昌职业大学博士启动金项目,