Vanadium-bearing steel slag,a secondary product generated during the smelting of vanadium-titanium magnetite,has an annual output approaching one million tonnes in China.In contrast to conventional steel slag,this material contains 1%–4%V2O5 in addition to ferrous components,conferring substantial potential for resource reclamation.Nevertheless,the intrinsic high-calcium and low-vanadium composition,coupled with the intricate mineralogical distribution of vanadium-bearing phases,poses significant challenges to existing treatment routes.For instance,electric arc furnace reduction entails considerable energy expenditure,whereas inorganic strong acid leaching suffers from inadequate selectivity,yielding leach liquors of complex composition and necessitating protracted downstream separation procedures.Although acetic acid-based treatment has been previously investigated,extant studies have predominantly focused on calcium dissolution and carbon sequestration,with limited systematic inquiry into the concurrent enrichment of vanadium and iron.This has hindered the development of an economically viable and technically effective processing strategy.Accordingly,there is an urgent imperative to establish a selective and benign methodology for the treatment of vanadium-bearing steel slag.In this study,acetic acid was employed as the lixiviant,and vanadium-bearing steel slag sourced from the Panxi region was utilized as the feedstock.The selective extraction of calcium-bearing constituents was conducted under ambient pressure,with the concomitant enrichment of vanadium and iron in the leach residue.A series of orthogonal experiments was designed to systematically evaluate the influences of particle size,liquid-to-solid ratio,acetic acid concentration,leaching temperature,and reaction duration on the dissolution behaviors of Ca,V,and Fe.The objective was to elucidate the selective dissolution mechanisms and to ascertain the optimal operating parameters that maximize calcium removal while minimizing vanadium and iron losses.Range analysis was applied to determine the relative significance of each factor affecting the leaching efficiencies of the three elements.Complementary characterization techniques,including X-ray diffraction(XRD),scanning electron microscopy(SEM),and X-ray photoelectron spectroscopy(XPS),were employed to examine the phase transformations and compositional modifications of the slag before and after leaching.The range analysis indicates that the factor effects on the leaching rates of the three elements exhibit distinct hierarchies.The calcium leaching rate is predominantly governed by the liquid-to-solid ratio(R=22.987),followed by acetic acid concentration(R=21.340).Similarly,the vanadium leaching rate is most strongly influenced by the liquid-to-solid ratio(R=21.177),with acetic acid concentration as the secondary determinant(R=14.823).In contrast,the iron leaching rate is primarily dictated by acetic acid concentration(R=5.778),and secondarily by particle size(R=4.47).With the objective of maximizing calcium extraction while minimizing vanadium and iron dissolution,the optimal conditions are identified as follows:particle size fraction of 38–48 μm,acetic acid concentration of 0.8 mol·L-1,liquid-to-solid ratio of 20 mL·g-1,ambient temperature(25℃),and reaction time of 40 minutes.Under these optimized parameters,the calcium leaching efficiency reaches 67.29%,whereas those of vanadium and iron are merely 9.22%and 5.69%,respectively.Correspondingly,the CaO content in the leach residue diminishes from 41.23%to 22.96%,while the V2O5 grade increases from 1.21%to 1.87%,and the total iron(TFe)grade rises from 24.39%to 39.16%.The enrichment ratios of vanadium and iron are determined to be 154.55%and 160.56%,respectively,thereby corroborating the selective removal of calcium and the efficient upgrading of vanadium and iron values.XRD analysis reveals that the diffraction peaks attributable to Ca2SiO4 and f-CaO are nearly eliminated following leaching,whereas those corresponding to Ca2Fe2O5,MgFe2O4,and RO phases exhibits no appreciable attenuation and,in some instances,slight intensification.This observation suggests that acetic acid preferentially dissolves Ca2SiO4 and f-CaO while exerting negligible attack on Ca2Fe2O5,MgFe2O4,and RO phases.SEM micrographs demonstrate a marked reduction in the spatial distribution of calcium and silicon within the leached residue.XPS spectra further corroborate a conspicuous weakening of calcium-related characteristic signals post-leaching,which is in good agreement with the XRD findings.In conclusion,the acetic acid-based selective leaching process proposes herein enables effective de-calcification of steel slag under mild,ambient-temperature conditions,while simultaneously facilitating the enrichment of vanadium and iron in the solid residue.The process exhibits favorable selectivity and operational simplicity.The resulting leach residue,characterized by elevated V2O5 and TFe grades,holds promise as a high-quality feed material for the smelting of vanadium-bearing pig iron.This work thereby offers a viable and technically sound pathway for the valorization of valuable elements present in vanadium-bearing steel slag.