军事知识服务平台
从冰铜渣中提取碲的工艺研究
Study on Technology of Extracting Tellurium from Matte Slag
摘要 碲是一种稀缺的战略稀散金属,在半导体、光电材料、冶金化工等领域应用广泛,市场需求量持续增长.工业生产中,冰铜渣作为铜冶炼过程的典型副产物,其中富集了大量未回收的碲资源,直接堆存不仅会造成稀有金属资源浪费,还易引发重金属流失、土壤及水体污染等环境问题.为实现冰铜渣资源化高效利用、提升稀散金属回收率,本文以铜冶炼冰铜渣为原材料,开展渣中碲的高效浸出与回收工艺研究.实验系统考察了浸出用酸浓度、反应温度、反应时间、二氧化锰添加量、液固体积比五大关键工艺参数对碲浸出率的影响,通过单因素试验优化确定最佳工艺条件.试验结果表明,最优工艺参数为浸出酸浓度8 mol·L-1、二氧化锰加入量0.30 g、液固比8:1 mL·g-1、反应温度40℃、反应时间30 min,此条件下碲浸出率可达95.3%±0.1%.将所得浸出液采用亚硫酸钠还原处理,碲最终回收率为93.40%.对还原产物进行XRD与SEM表征分析,结果显示产物为分散性良好的球状单质碲颗粒,碲特征衍射峰尖锐且显著,产物纯度与物相特征良好.本研究优化的工艺简单高效,可为冶炼废渣中碲的绿色回收与工业化应用提供可靠的理论依据和技术支撑.
Abstract:
Tellurium is a strategically scarce dispersed metal in China,with excellent photovoltaic,thermal conductivity and semiconductor properties.It is the core raw material for manufacturing photovoltaic cells,thermal sensitive components,high-end metallurgical alloys and chemical catalysts.With the rapid development of new energy and high-end new materials industries,the domestic supply-demand gap of tellurium resources has been continuously expanding,and the scarcity of resources has become increasingly prominent.In the copper hydrometallurgical industrial system,ice copper slag is a solid by-product with a large output.During the smelting process,most of the tellurium elements are concentrated in the ice copper slag.If it is directly buried or stored,it will not only cause the permanent loss of high-value tellurium resources,but also significantly reduce the comprehensive utilization rate of mineral resources.Moreover,due to the weathering and dissolution of heavy metals and valuable components in the waste residue,it will cause environmental pollution of the surrounding soil and groundwater,posing serious ecological hazards.Therefore,conducting research on the efficient extraction and recovery of tellurium from ice copper slag has important practical significance and engineering value for achieving the resource utilization and recycling of industrial solid waste,energy conservation and emission reduction,and alleviating the shortage of dispersed metal resources.This paper uses copper smelting waste ice copper slag as the test raw material and adopts an acid leaching-reduction combined process to recover the tellurium resources in the slag.The optimal parameter system of the wet extraction process is mainly explored.Through the single-factor variable method,the influence laws of five core process conditions,including acid concentration for leaching,reaction temperature,holding time,manganese dioxide oxidant addition amount,and liquid-solid volume ratio,on the leaching effect of tellurium were systematically studied.The various process parameters were precisely optimized.The test results show that the optimal extraction process conditions are:acid concentration of 8 mol·L-1,manganese dioxide addition amount of 0.30 g,liquid-solid ratio of 8:1 mL·g-1,reaction temperature of 40℃,and constant temperature leaching time of 30 min.Under this suitable condition,the leaching rate of tellurium in the ice copper slag is stable at 95.3%±0.1%,and the leaching effect is excellent.Subsequently,the high-purity leaching solution was treated by sodium sulfite for reduction purification,and the total recovery rate of tellurium was 93.40%.To clarify the phase structure and microscopic morphology of the reduction product,XRD analysis and SEM scanning electron microscope characterization tests were carried out on the obtained product.The test results show that the reduction product is elemental tellurium,with regular spherical particles,uniform dispersion,and no obvious agglomeration phenomenon.The characteristic diffraction peaks of the sample tellurium are sharp and highly identifiable,and are highly consistent with the standard elemental tellurium phase diagram.The product has high purity and good crystallization performance.The tellurium extraction process constructed in this study has the advantages of mild conditions,low energy consumption,high recovery rate,and excellent product quality.It effectively solves the problems of low efficiency and high impurity content in traditional waste residue tellurium extraction processes,and can provide solid experimental data and technical references for the green and efficient industrial recovery and utilization of rare earth metal tellurium in copper smelting waste residues.
刊 名 有色金属(中英文) ISTICPKU
年,卷(期): 2026, 16(10)
分类号: TF843
机标分类号: TF811 X52 X758
在线出版日期: 2026年10月28日