The corrosion behavior of Ti-0.3Mo-0.8Ni-0.01Y sheets after annealing at different temperatures is investigated to clarify how annealing-induced α/β microstructural evolution affects the electrochemical response and immersion corrosion behavior in a reducing acid environment.Ti-0.3Mo-0.8Ni is a near-α corrosion-resistant titanium alloy used in chloride-containing and acidic service conditions,but its corrosion response is sensitive to the morphology and distribution of α and β phases generated during thermomechanical processing and subsequent heat treatment.In this study,hot-rolled Ti-0.3Mo-0.8Ni-0.01Y sheets were annealed at 670,770 and 870℃for 2 h,followed by air cooling.The annealing temperatures were selected according to the phase transformation behavior determined from DSC/DDSC analysis,in which the α/(α+β)and(α+β)/β transformation temperatures are 691.8℃and 878.6℃,respectively.The microstructure and phase constitution were characterized by optical microscopy and X-ray diffraction,while the corrosion behavior was evaluated by open-circuit potential measurement,potentiodynamic polarization,electrochemical impedance spectroscopy,immersion weight-loss testing and scanning electron microscopy after immersion in 5 mol·L-1 HCl solution.The results show that annealing temperature changes the α/β microstructure of the Ti-0.3Mo-0.8Ni-0.01Y sheets.The 670℃annealed sample exhibits a mixed microstructure consisting of equiaxed grains and elongated or strip-like features,indicating that recovery and partial equiaxed microstructural evolution occur during low-temperature annealing.The 770℃annealed sample shows a more equiaxed and relatively uniform microstructure,suggesting enhanced microstructural evolution in the α+β region.When the annealing temperature increases to 870℃,the alloy develops a basket-weave Widmanstätten microstructure containing lamellar α/β features,which is associated with annealing near the(α+β)/β transformation temperature and subsequent cooling.XRD patterns indicate that the hot-rolled and annealed samples are mainly composed of α-Ti and a small amount of β-Ti.No additional phase is confirmed by the current XRD results;Therefore,the corrosion mechanism is discussed primarily in terms of α/β microstructural morphology rather than unverified Y-containing second phases.Electrochemical measurements reveal that the annealed samples exhibit different surface responses in 5 mol·L-1 HCl solution.The open-circuit potentials(OCP)of the A670 and A770 samples are relatively stable and finally stabilize at approximately –0.17 V and –0.18 V,respectively,whereas the A870 sample shows a pronounced negative shift and stabilizes at approximately–0.46 V.This indicates that the surface electrochemical state of the A870 sample changes more strongly in the acidic chloride environment.The polarization curves show similar cathodic behavior among the samples and reveal active dissolution,active-passive transition and passive-like regions in the anodic branches,suggesting competition between surface film formation and dissolution during polarization.The EIS results provide a more quantitative comparison of the interfacial response.The A670 sample shows the highest fitted film resistance,with Rf=77060 Ω·cm2.The A770 sample has Rf=1548 Ω·cm2 and Rct=45890 Ω·cm2,whereas the A870 sample shows much lower values,with Rf=401.4 Ω·cm2 and Rct=1421 Ω·cm2.These results indicate that the A670 sample has the strongest impedance response among the tested conditions,while the A870 sample exhibits the weakest interfacial blocking ability.Immersion weight-loss testing in 5 mol·L-1 HCl at(35±1)℃further confirms the electrochemical trend.The corrosion rates of the A670,A770,A870 and HR samples are 2.245 92,2.699 268,3.213 27 and 2.670 71 mm·a-1,respectively.The A670 sample exhibits the lowest corrosion rate,whereas the A870 sample shows the highest corrosion rate.SEM observations after immersion show that localized dissolution occurs on all samples,but the corrosion damage becomes more pronounced for the A870 sample.After longer immersion,the A870 surface contains larger and more connected corrosion regions than the lower-temperature annealed samples.The inferior corrosion resistance of the A870 sample is likely associated with its lamellar α/β morphology,which may increase the continuity of α/β interfaces and enhance local electrochemical heterogeneity in 5 mol·L-1 HCl solution.However,this interpretation is correlation-based;direct proof of micro-galvanic corrosion would require additional local compositional or electrochemical evidence.Overall,the present results demonstrate that annealing temperature is a key processing parameter for regulating the α/β microstructure and corrosion response of Ti-0.3Mo-0.8Ni-0.01Y sheets in hydrochloric acid.