军事知识服务平台
热暴露温度对添加(Al-Ti-La+Nd)的Al-7Si-0.35Mg合金热稳定性的影响
Effect of Thermal Exposure Temperature on the Thermal Stability of Al-7Si-0.35Mg Alloy with(Al-Ti-La+Nd)Addition
摘要 为探究热暴露温度对复合细化变质协同T6处理后的Al-7Si-0.35Mg合金显微组织与力学性能的影响,本研究向合金中复合添加0.3 wt.%Al-3Ti-4.35La与0.03 wt.%Nd,经T6热处理后,在100~300℃范围内进行热暴露处理.结果表明:当热暴露温度低于200℃时,合金显微组织稳定性良好,α-Al枝晶无明显粗化,共晶Si保持球状分布,析出表面富集La和Nd的二次Si相有效抑制了Si相的长大,力学性能降幅较小;当温度超过200℃时,α-Al枝晶显著粗化,共晶Si发生严重偏聚与黏连,二次Si相长大加剧,导致力学性能急剧恶化.研究证实,复合添加Al-3Ti-4.35La与Nd可显著提升Al-7Si-0.35Mg合金在200℃左右的热稳定性,为该合金在高温服役条件下的应用提供了理论依据和技术支撑.
Abstract:
With the rapid development of the automotive industry towards high performance and lightweighting,Al-Si-Mg alloys have been widely utilized owing to their merits of low density,high specific strength and favorable formability.Nevertheless,Al-Si-Mg alloys are susceptible to microstructure coarsening and degradation of mechanical properties in high-temperature environments,which severely restricts their application scope under medium and high temperatures.Therefore,this study aims to improve the high-temperature thermal stability of Al-7Si-0.35Mg alloy through composite refinement-modification synergized with T6 treatment,so as to meet the service demands of key components including automotive engine pistons and cylinder blocks under long-term high-temperature working conditions.Commercially pure aluminum,Al-20Si master alloy and pure magnesium were adopted as matrix materials,and the burdening was implemented in accordance with the composition design of Al-7Si-0.35Mg.Melting was conducted in a graphite crucible via a resistance furnace.To realize the synergistic effect of grain refinement and modification of the alloy,0.3 wt.%Al-3Ti-4.35La master alloy and 0.3 wt.%Al-10Nd master alloy were added into the melt.After thorough stirring,standing and degassing,the melt was cast into a permanent mold preheated to 200℃to fabricate alloy specimens.Subsequent to specimen preparation,the T6 heat treatment process was performed:solution treatment at 510℃for 4 h was conducted first,followed by water quenching at 60℃,and finally aging treatment at 165℃for 3 h to optimize the mechanical properties of the alloy.To simulate the high-temperature service environment of the alloy in practical applications,the T6-treated alloy specimens were placed in a KSL-1200 muffle furnace and subjected to thermal exposure at five temperature gradients of 100,150,200,250 and 300℃respectively for 1 h.Optical Microscopy(OM),Scanning Electron Microscopy(SEM)and Energy Dispersive Spectroscopy(EDS)were employed to systematically characterize the evolution law of the alloy microstructure at different thermal exposure temperatures.The room-temperature tensile properties of the alloy were tested by a universal material testing machine in compliance with the GB/228.1-2010 standard,and the influences of thermal exposure temperature on the Ultimate Tensile Strength(UTS),Yield Strength(YS)and elongation of the alloy were analyzed.The experimental results demonstrate that the composite addition of(Al-3Ti-4.35La+Nd)combined with T6 heat treatment can effectively enhance the thermal stability of Al-7Si-0.35Mg alloy at a service temperature of around 200℃.Its mechanical properties are significantly correlated with the thermal exposure temperature and highly consistent with the evolution law of the microstructure.When the thermal exposure temperature is below 200℃,the alloy maintains favorable stability in mechanical properties:the Ultimate Tensile Strength(UTS)remains at approximately 268.2 MPa,and the Yield Strength(YS)is about 160.5 MPa,with reduction rates of merely 6.7%and 7%respectively.This is attributed to the fact that the Ti2Al20La phase,acting as heterogeneous nucleation sites,effectively restrains the coarsening trend of α-Al dendrites during thermal exposure.Meanwhile,the enrichment of rare earth elements La and Nd on the surfaces of eutectic Si phase and secondary Si phase inhibits their growth and morphological deterioration.However,when the thermal exposure temperature exceeds 200℃,the microstructure and mechanical properties of the alloy deteriorate drastically.Obvious coarsening of α-Al dendrites emerges at 250℃,and the Secondary Dendrite Arm Spacing(SDAS)even reaches 20.3 μm at 300℃.Severe segregation and coalescence occur in the eutectic Si phase,which intensifies the internal stress concentration effect of the alloy and promotes the initiation and propagation of cracks in the Si phase aggregation regions.Correspondingly,after thermal exposure at 300℃,the UTS and YS of the alloy decrease to 124.8 MPa and 38.4 MPa respectively,with a reduction rate exceeding 30%.Comparative experiments reveal that compared with the conventional Al-Ti-B+Sr modification treatment,the(Al-3Ti-4.35La+Nd)composite treatment effectively retards the coarsening rate of α-Al dendrites and the segregation and coalescence of eutectic Si phase at high temperatures through the synergistic effect of refinement and modification.It raises the effective service temperature of Al-7Si-0.35Mg alloy from about 150℃of the traditional process to approximately 200℃,significantly expanding its application temperature range.The findings of this study provide an important theoretical basis and practical technical support for the application of Al-7Si-0.35Mg alloy in high-temperature working conditions such as the automotive industry,and also put forward a novel compositional design strategy for aluminum alloy components serving at medium and high temperatures.
刊 名 有色金属(中英文) ISTICPKU
年,卷(期): 2026, 16(10)
分类号: TG146.21
机标分类号: TG115 TG457.1 TP391
在线出版日期: 2026年10月28日